Coppell Trade-LR051013CONCRETE COMPRESSIVE STRENGTH TEST
Report Number: 94051190.0126
Service Date: October 5, 2005
Client:
Coppell Trade Center LP
Attn: Bennet Ratliff
5055 Keller Springs Rd Ste 300
Addison TX 75001
Report Date: October 13, 2005
Project:
'1 rerracon
8901 Carpenter F~vy, Ste #100
Dallas, Texas 75247
(214) 630-1010
Coppell Trade Center - Bldg C
NWC Sandy Lake/Freepod Pkwy
Coppell, TX
Project No.: 94051190
Material Information
Specified Strength: 4000 psi @ 28 Days
Batch Time: 10:35am
Supplier: TXI
Truck No: 69
Mix I.D. No.: 8206
Water Added Onsite Before Test:
Water Added Onsite After Test:
Field Test Data
Test Result
Slump, inches: 5.00
Air Content, %: 5.0
Concrete Temperature,° F: 93
Ambient Temperature, o F: 83
Plastic Unit Weight, pcf: 144
Laboratory Test Data
Set specimen Diameter Area
No. ID (inches) (sq. inches)
1 1 6.00 28.27
Plant: 141
Ticket No: 131463
0 Gallons
0 Gallons
Sample Information
sample Time: 11:02am Date Cast: October 5, 2005
Technician: Burl E. Thomas
Weather Conditions: Hazy
Accumulative Yards: 20
Placement Method: Direct Discharge
Sample Locations: 3' W & 150' S of Building, NW comer
Placement Location: Pavement, W of Building
Specification
Test Method
3-5 ASTM C143
4-6 ASTM C231
ASTM C1064
ASTM C1064
ASTM C138
Age at Maximum Compressive
Date Test Load Strength
Tested (days) (lbs) (psi)
10/12/2005 7 89,710 3,170
1 2 11/02/2005 28
1 3 11/02/2005 28
Services - Obtain samples of fresh concrete at the placement locations, perform required field tests and cast compressive
strength samples.
Technician: Burl E. Thomas
Report Distribution:
(1) Coppell Trade Center LP (1) Merdman Assoc In(;
(1) TechniStructures (1) McFadden & Miller Reviewed by:
(1) City of Coppell TX (1) Macatee Engineering
(1) City of Coppell TX Robert D. Ray, S/~.
Senior P r oJ~t~a'nage r ..
The tests were performed in general accordance with applicable ASTM, AASHTO, or DOT test methods. This ra~ for the u§e of the client
indicated above and shall not be reproduced except in full without the written consent of our company. Test results transmitted herein are only applicable
to the actual samples tested at the location(s) referenced and are not necessarily indicative of the properties of other apparently similar or identical
materials.