Coppell Trade-LR060227CONCRETE COMPRESSIVE STRENGTH TEST
Report Number: 94051190.0200
Service Date: January 27, 2006
'lrerracon
8901 Carpenter Frwy, Ste #100
Dallas, Texas 75247
(214) 630-1010
Client:
Coppell Trade Center LP
Attn: Bennet Ratliff
5055 Keller Springs Rd Ste 300
Addison TX 75001
Material Information
Specified Strength: 4000 psi ~ 28 Days
Batch Time: 6:48am Plant: 141
Supplier: TXI
Truck No: 102 Ticket No: 196067
Mix I.D. No.: 8206
Water Added Onsite Before Test: 0Gallons
Water Added Onsite After Test: 0 Gallons
Report Date: Februa~,Q~27, 2006
Project: ~jT,~e~Sell Trade Center- B[d~,,~J~
f Nwc sanuy Lake/ j -% rPk
- Coppell, TX ~J
Project No.: 94051190 ~,/' "~J
Sample Information
Date Cast: January 27, 2006 Time: 7:30am
Technician: Kudret Aksu ~'~
Weather Conditions: Clear ~ o ~ · ~
Accumulative Yards: 20/90
Placement Method: Pump
Sample Locations: SW corner of Placement Are,
Placement Location: Pavement, SW corner of Building, next to
Ramp Retaining Wall
Field Test Data
Test
Specification
3-5
3-6
Result
Slump, inches: 5.00
Air Content, %: 4.8
Concrete Temperaturep F: 59
Ambient Temperature,o F: 46
Plastic Unit Weight, pcf: 144.2
Laboratory Test Data
Set Specimen Diameter Area
No. ID (inches) (sq. inches)
1 1 6.00 28.27 02/03/2006
1 2 6.00 28.27 02/03/2006
1 3 6.00 28.27 02/24/2006
1 4 6.00 28.27 02/24/2006
Date
Tested
Test Method
ASTM C143
ASTM C231
ASTM C1064
ASTM C1064
ASTM C138
Age at Maximum Compressive
Test Load Strength
(days) (lbs) (psi)
7 122,170 4,320
7 125,150 4,430
Average (7 Days) 4,380
28 160,930 5,690
28 161,240 5,700
Average (28 Days) 5,700
Services - Obtain samples of fresh concrete at the placement locations, perform required field tests and cast compressive
strength samples.
(1) Coppell Trade Center LP (1) Merriman Assoc [nc
(1) TechniStructures (1) McFadden & Miller Reviewed by:
(1) City of Coppell TX (1) Macatee Engineering Inc ~' -- Robert D. Ray, S.E.T~~
(1) City of Coppell TX Senior Project Ma~er~'
The tests were performed in general accordance with applicable ASTM, AASHTO, or DOT test methods. This report is exclusively for the use df the client
indicated above and shall not be reproduced except in full without the written consent of our company. Test results transmitted herein are only applicable
to the actual samples tested at the location(s) referenced and are not necessarily indicative of the properties of other apparently similar or identical
materials.